19% TO 82% BETTER SHEAR STABILITY

    ROLL STABILITY TEST (ASTM D-1831)


  • In this test a sample of grease is worked for 60 strokes and its penetration is measured in accordance with the ASTM D-1403 “Test For Cone Penetration of Lubricating Grease Using One-Quarter and One- Half Scale Cone Equipment”.

  • After the worked penetration is determined and recorded a 50 gram sample of grease that has not been worked is placed in the test cylinder and distributed uniformly on the inside wall of the cylinder.

  • A weighted roll is placed inside the cylinder , the cap tightened and the entire cylinder assembly is mounted onto the test assembly.

  • The test assembly is started and the weighted roll revolves along the inside of the cylinder at 165 rpm for a period 2 hours.

  • At the end of a two hour rolling period the cylinder assembly is dismantled and the grease being tested is removed so that its worked penetration according to the ASTM D-1403 can be determined.

  • From the before and after penetration readings the percent change in consistency is calculated.